Ubicación: Global + English
Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Coating Film Flexibility Testing to Chinese National Standards (GB/T): Methods, Procedures and Appli

Coating film flexibility is a critical mechanical property that determines whether a paint film can withstand bending, forming, and substrate deformation without cracking or peeling. In China, this property is evaluated using national standard test methods such as GB/T 1731 and GB/T 6742, which are mandrel bend tests widely applied in coating quality control, product certification, and R&D. This article provides a comprehensive technical overview of national standard flexibility testing for coating films, covering applicable sample types, test items, detailed procedures, and typical industrial applications.

Technical Overview

Coating film flexibility refers to the ability of a dry paint film, together with its substrate, to undergo bending deformation without cracking, flaking, or losing adhesion. It is one of the fundamental mechanical performance indicators for paints and varnishes, alongside adhesion, impact resistance, and hardness. Films with poor flexibility will crack when the coated object is bent, formed, transported, or exposed to thermal expansion and contraction, leading to corrosion initiation and premature coating failure.

In the Chinese national standard system, coating film flexibility is primarily evaluated by mandrel bend tests. The two core national standards are:

  • GB/T 1731 — Determination of flexibility of paint films. This classic national method uses a multi-mandrel flexibility tester (a base-mounted set of steel rods of graded diameters) and expresses the result as the smallest mandrel diameter over which the film passes a 180-degree bend without damage.
  • GB/T 6742 — Paints and varnishes — Bend test (cylindrical mandrel). This standard is technically aligned with ISO 1519 and uses a single cylindrical mandrel bending device to assess pass/fail performance at a specified mandrel diameter or to determine the minimum passing diameter.

For international equivalence, results from these methods can be correlated with ISO 1519 (cylindrical mandrel bend), ISO 6860 (conical mandrel bend), and ASTM D522 (mandrel bend test of attached organic coatings). Related national standards frequently tested in combination include GB/T 9286 (cross-cut adhesion test, corresponding to ISO 2409), GB/T 1732 (impact resistance), and GB/T 9753 (cupping test). All of these tests can be performed by accredited third-party laboratories or in-house quality control departments.

Testing Samples

Laboratory-Prepared Coated Panels

For liquid coating products (such as alkyd paints, amino paints, acrylic coatings, epoxy systems, and waterborne architectural coatings), test panels are prepared in the laboratory. The coating is applied by spray, dip, draw-down bar, or film applicator onto standardized substrates — most commonly tinplate panels of approximately 25 mm x 120 mm and 0.2 mm to 0.3 mm thickness for GB/T 1731, or soft metal panels (steel, tinplate, or aluminum) of suitable dimensions for GB/T 6742. The film is then dried or cured under the temperature and time conditions specified in the product standard, and the dry film thickness is verified (for example, in accordance with GB/T 13452.2).

Production-Coated Sheets and Parts

For coil coatings, pre-painted metal sheets, powder-coated components, and factory-finished parts, specimens can be cut directly from production material, provided the panel size, flatness, and thickness meet the requirements of the selected test method. The coating must be fully cured and free of surface contamination before testing.

Conditioning Requirements

Prior to testing, samples are normally conditioned in a standard atmosphere of 23 ± 2 °C and 50 ± 5 % relative humidity for a defined period (commonly 16 hours to 24 hours, or as specified in the product standard). Temperature control is essential because coating films become more brittle at low temperatures and softer at elevated temperatures, which directly affects bend test results.

Testing Items

The typical test items covered under national standard flexibility testing include:

  • 180-degree mandrel bend flexibility of the paint film (GB/T 1731 multi-mandrel tester).
  • Cylindrical mandrel bend test at a specified diameter, pass/fail determination (GB/T 6742 / ISO 1519).
  • Determination of the minimum mandrel diameter at which no cracking or detachment occurs.
  • Post-bend visual assessment of film integrity: checking for cracking, checking, flaking, peeling, and loss of adhesion.
  • Combined evaluation with complementary mechanical properties such as cross-cut adhesion (GB/T 9286), impact resistance (GB/T 1732), and cupping (GB/T 9753), where required by the product specification.

Acceptance criteria are defined in the relevant product standards. For example, many general-purpose paints require passing a 1 mm or 2 mm mandrel, while decorative or industrial coatings may specify 2 mm to 10 mm depending on the intended service and substrate.

Testing Methods

Apparatus

The GB/T 1731 flexibility tester consists of a set of polished steel mandrels of graded diameters (typically 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, and 10 mm, depending on the instrument configuration) rigidly mounted on a common base. The GB/T 6742 apparatus uses a single cylindrical mandrel with an associated bending lever and clamping device; interchangeable mandrels commonly range from 2 mm up to 32 mm in diameter. Mandrel surfaces must be smooth, free of defects, and cleaned between tests.

Procedure

The general test procedure is as follows:

  • Prepare and cure the coated panel according to the product standard, and condition it in the standard atmosphere.
  • Select the mandrel diameter to be tested. When determining the minimum passing diameter, testing usually begins with the largest mandrel and proceeds to progressively smaller diameters, or vice versa as specified.
  • Place the coated panel with the film facing outward over the mandrel and bend the panel smoothly through 180 degrees around the mandrel within approximately 1 to 3 seconds, using steady pressure. The bending operation should be completed in one continuous motion.
  • Immediately after bending, examine the film at the bend region with normal corrected vision (a 10x magnifier may be used where specified) for cracking, flaking, or detachment from the substrate.
  • Record the result: either the smallest mandrel diameter at which the film remains intact, or pass/fail at the specified diameter.

Expression of Results

Under GB/T 1731, flexibility is expressed as the minimum mandrel diameter in millimeters over which the film passes without visible damage — a smaller value indicates better flexibility. Under GB/T 6742, the result is typically reported as pass or fail at a single specified mandrel diameter, or as the minimum passing diameter when a graded series is used. The test report should identify the standard used, mandrel diameter(s), film thickness, substrate type, conditioning conditions, bending speed, number of replicates, and any observed failure mode.

Key Influencing Factors

  • Dry film thickness: thicker films generally exhibit poorer bend performance.
  • Test temperature and humidity: low temperature increases brittleness and the risk of cracking.
  • Curing degree: under-cured or over-baked films may show reduced flexibility.
  • Bending speed: excessive speed can introduce impact effects and false failures.
  • Substrate thickness and type: substrate properties influence strain distribution at the bend.

Applications

National standard flexibility testing is applied throughout the coatings industry and related sectors:

  • Architectural and decorative coatings: verifying that emulsion paints and enamels on wood, plaster, and metal substrates can tolerate minor building movement without cracking.
  • Industrial anti-corrosion coatings: evaluating epoxy, polyurethane, and alkyd systems used on steel structures, storage tanks, and pipelines where flexing and vibration occur.
  • Coil coatings and pre-painted metals: confirming that coil-coated sheets survive roll forming, profiling, and fabrication after coating application.
  • Automotive and transportation coatings: supporting formulation development and quality control of primers and topcoats that must endure panel deformation and stone impact.
  • Wood coatings and furniture finishes: ensuring lacquers and varnishes accommodate the natural expansion and contraction of wood substrates.
  • Packaging and can coatings: assessing interior and exterior can linings that must withstand flanging, necking, and other metal-forming operations.
  • Product certification and compliance: providing test evidence for factory acceptance, tender submissions, and conformance declarations to national and international specifications, often issued through accredited third-party laboratories.
  • Research and development: comparing resin systems, pigment volume concentration, and additive packages during coating formulation optimization.

FAQ

What does a flexibility result of 1 mm mean?

It means the coating film passed a 180-degree bend around a 1 mm diameter mandrel without cracking or peeling. A smaller mandrel diameter corresponds to greater elongation of the film at the bend, so smaller values indicate superior flexibility.

What is the difference between GB/T 1731 and GB/T 6742?

GB/T 1731 is the traditional Chinese national method using a multi-mandrel flexibility tester and reports the minimum passing diameter. GB/T 6742 is aligned with ISO 1519 and uses a cylindrical mandrel bending apparatus, typically for pass/fail assessment at a specified diameter or for minimum diameter determination. Both are bend tests, but they differ in apparatus design, panel dimensions, and reporting convention.

Which substrates and panel sizes are used?

Tinplate panels of approximately 25 mm x 120 mm with a thickness of 0.2 mm to 0.3 mm are typical for GB/T 1731. GB/T 6742 generally uses soft metal panels cut to dimensions compatible with the bending device, with substrate thickness preferably below 1.0 mm so that bending occurs around the mandrel rather than through the panel.

How should samples be conditioned before testing?

Samples are normally conditioned at 23 ± 2 °C and 50 ± 5 % relative humidity for at least 16 hours, unless the product standard specifies otherwise, and testing should be carried out under similar conditions to ensure reproducibility.

How is the film examined after bending?

The bent area is inspected immediately after bending with normal corrected vision, or with a 10x magnifier where the standard requires, for cracking, checking, flaking, or detachment. Any visible film failure at the bend constitutes a failure at that mandrel diameter.

Can these national standard results be compared with international standards?

Yes. GB/T 6742 corresponds technically to ISO 1519, and conical mandrel or cylindrical mandrel methods under ISO 6860 and ASTM D522 are widely used internationally. Accredited third-party laboratories can perform testing to GB, ISO, and ASTM specifications and help correlate results for global market acceptance.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing