Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Intergranular Corrosion Test Methods for Stainless Steel: Standards, Practices, and Evaluation

Intergranular corrosion (IGC) testing is an essential quality control procedure used to evaluate the resistance of stainless steels to grain boundary attack caused by sensitization, chromium carbide precipitation, and sigma phase formation. This technical article reviews the standardized intergranular corrosion test methods for stainless steel—including the oxalic acid etch test, ferric sulfate–sulfuric acid test, boiling nitric acid (Huey) test, nitric–hydrofluoric acid test, and copper–copper sulfate–sulfuric acid (Strauss) test—in accordance with internationally recognized standards such as ASTM A262, ASTM A763, ISO 3651, GB/T 4334, and JIS G 0571–G 0575.

Technical Overview

Intergranular corrosion is a localized form of attack that proceeds along the grain boundaries of a metal while the bulk grains remain largely unaffected. In stainless steels, this phenomenon is most commonly associated with sensitization: when the material is heated within the critical temperature range of approximately 425 °C to 815 °C (800 °F to 1500 °F), chromium combines with carbon to precipitate chromium-rich carbides (typically M23C6) at the grain boundaries. This depletes the adjacent zones of chromium to below the level required for passivation (roughly 12%), leaving them vulnerable to preferential corrosion in aggressive media. Similar susceptibility can be introduced by sigma phase precipitation or by the thermal cycles experienced during welding in the heat-affected zone (HAZ).

Because intergranular attack can cause grain dropping, severe loss of ductility and strength, and ultimately catastrophic failure with little external warning, standardized laboratory methods have been developed to detect susceptibility before components enter service. These methods fall into two categories: rapid electrochemical screening tests based on electrolytic etching, and quantitative immersion tests that measure corrosion rates or post-exposure ductility. The principal standards governing such testing include:

  • ASTM A262 – Standard Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels (Practices A, B, C, E, F)
  • ASTM A763 – Standard Practices for Detecting Susceptibility to Intergranular Attack in Ferritic Stainless Steels (Practices W, X, Y, Z)
  • ISO 3651-1 and ISO 3651-2 – Determination of resistance to intergranular corrosion of stainless steels (austenitic, ferritic-austenitic, and ferritic grades)
  • GB/T 4334 series – Chinese national standard covering the oxalic acid, ferric sulfate–sulfuric acid, nitric acid, nitric–hydrofluoric acid, and sulfuric acid–copper sulfate test methods
  • JIS G 0571 to G 0575 – Japanese industrial standards corresponding to the five classical test media
  • ASTM G28 – Detecting susceptibility to intergranular corrosion in wrought nickel-rich, chromium-bearing alloys

Testing Samples

Test specimens must be representative of the product form, metallurgical condition, and, where applicable, the welded region to be evaluated. Accredited third-party laboratories typically prepare coupons with fully exposed, identified surfaces and record the exact exposed area for corrosion rate calculations.

Flat-Rolled Products (Plate, Sheet, and Strip)

Coupons are cut with sufficient surface area to satisfy the minimum solution-volume-to-area ratio required by the governing standard. Mill scale, decarburized layers, and heat-treatment oxides are removed by grinding or pickling, and the surfaces are degreased, rinsed, dried, and weighed to the required precision.

Bars, Rods, Forgings, and Castings

Specimens are machined from the section in the orientation specified by the product specification. Castings may require additional surface conditioning to remove the cast skin, and heavy sections are sampled at locations agreed between the purchaser and supplier.

Pipes and Tubes

Test pieces may consist of full ring segments or longitudinally cut strips, with the cut edges ground smooth. For welded pipes, specimens are oriented so that the weld metal, fusion line, and heat-affected zone are all exposed to the test medium.

Welded Joints and Weldments

Cross-section coupons containing base metal, weld metal, and HAZ are exposed as a single specimen so that sensitized zones created by the welding thermal cycle are directly evaluated. As-welded specimens are tested without additional heat treatment unless otherwise specified.

Specimen Conditioning and Sensitizing Heat Treatment

When the intrinsic susceptibility of a grade must be assessed—for example, for low-carbon or stabilized steels in the solution-annealed delivery condition—a sensitizing treatment is applied before exposure. Common treatments include 650 °C for 2 hours followed by air cooling, or 700 °C for 30 minutes followed by water quenching as specified in ISO 3651. The exact conditioning is always defined by the material specification or purchase agreement.

Testing Items

The core scope of an intergranular corrosion test program for stainless steel typically includes:

  • Susceptibility to intergranular attack in electrolytic etch (screening) examination
  • Corrosion rate determination by gravimetric mass loss after immersion testing
  • Bend ductility evaluation of specimens after acid exposure (fissure/crack detection)
  • Evaluation of sensitization from welding thermal cycles in the heat-affected zone
  • Detection of chromium carbide precipitation and sigma phase contribution to attack
  • Verification of the effectiveness of solution annealing and stabilization treatments

Acceptance criteria—such as maximum permissible corrosion rates or the absence of fissures after bending—are established by the governing product specification, the applicable code, or agreement between the purchaser and supplier.

Testing Methods

The classical test media differ in aggressiveness, target microstructural features, and evaluation technique. Selection depends on the steel grade, product form, service environment, and the relevant specification.

Oxalic Acid Etch Test (ASTM A262 Practice A / GB/T 4334.1 / JIS G 0571)

A 10% oxalic acid solution is used as the electrolyte at room temperature. The polished specimen is made the anode and etched at a current density of 1 A/cm² for 90 seconds. The etched microstructure is then examined at 250× to 500× magnification and classified as:

  • Step structure – steps between grains without ditches; indicates resistance for most grades
  • Dual structure – ditches at some boundaries but no grain completely surrounded; conditionally acceptable depending on grade and practice
  • Ditch structure – one or more grains completely enclosed by ditches; indicates susceptibility and requires confirmation by an immersion test

This rapid, low-cost method is a screening test only and is not used alone for final acceptance. It is classified as a qualitative quality control tool because the etched surface is consumed during examination.

Ferric Sulfate–Sulfuric Acid Test (ASTM A262 Practice B / GB/T 4334.2 / JIS G 0572)

Specimens are immersed for 120 hours in a boiling solution of 50% sulfuric acid containing 25 g/L ferric sulfate, using a reflux condenser to maintain constant concentration. Attack is quantified by mass loss, and the ferric/ferrrous redox couple accelerates the corrosion of chromium-depleted regions. The test detects susceptibility associated with chromium carbide precipitation and, for certain grades, sigma phase.

Boiling Nitric Acid (Huey) Test (ASTM A262 Practice C / GB/T 4334.3 / JIS G 0573 / ISO 3651-1)

The specimen is exposed to boiling 65% nitric acid for five consecutive 48-hour periods (240 hours total), with fresh solution for each period and mass loss measured after every cycle. Because hot nitric acid also attacks sigma phase, chromium-depleted zones, and certain inclusions, this is the most discriminating and severe of the classical tests. Results are reported as the corrosion rate for each period and the average, with acceptance limits set by the product specification.

Nitric–Hydrofluoric Acid Test (GB/T 4334.4 / JIS G 0574 / Former ASTM A262 Practice D)

This method is intended primarily for molybdenum-bearing austenitic grades such as 316 and 316L. Specimens are immersed in a 10% nitric acid plus 3% hydrofluoric acid solution at 70 °C for two consecutive 2-hour periods with fresh solution each time. Because the medium is highly aggressive even to properly annealed material, evaluation is based on the ratio of the specimen corrosion rate to that of a known-resistant reference specimen tested in parallel; ratios exceeding the specified limit (commonly 1.5) indicate susceptibility.

Copper–Copper Sulfate–Sulfuric Acid (Strauss) Test (ASTM A262 Practice E / GB/T 4334.5 / JIS G 0575 / ISO 3651-2)

Specimens are placed in contact with metallic copper chips in a boiling solution of copper sulfate in approximately 16% sulfuric acid. Exposure is 24 hours in ASTM A262 and a minimum of 20 hours in ISO 3651-2. After exposure, each specimen is bent through 180° around a mandrel of appropriate diameter and examined at low magnification (typically 5× to 20×) for cracks and fissures. The presence of intergranular fissures indicates sensitization. This widely specified test is particularly relevant to environments containing sulfur-bearing species.

Copper–Copper Sulfate–50% Sulfuric Acid Test (ASTM A262 Practice F)

Designed for molybdenum-bearing austenitic stainless steels such as 316 and 317, this 24-hour boiling test uses a more aggressive medium than Practice E to reveal grain boundary attack in grades whose molybdenum content otherwise reduces the sensitivity of the standard Strauss solution. Evaluation is performed by the same bend-test procedure.

Ferritic Stainless Steels (ASTM A763)

For ferritic grades, ASTM A763 provides Practices W, X, Y, and Z, which combine electrolytic etch screening with immersion testing in ferric sulfate–sulfuric acid or copper–copper sulfate–sulfuric acid media. The applicable practice is selected according to alloy composition, particularly the molybdenum content, and the acceptance criteria specified for the grade.

Result Evaluation and Corrosion Rate Calculation

For immersion tests, corrosion rates are calculated from mass loss using the relationship:

Corrosion rate (mm/y) = (8.76 × 10⁴ × W) / (A × T × D), where W is the mass loss in grams, A is the exposed surface area in cm², T is the exposure time in hours, and D is the density in g/cm³ (approximately 7.9–8.0 g/cm³ for austenitic stainless steels). The equivalent expression in mils per year uses a factor of 3.45 × 10³. For bend-evaluated tests, the acceptance criterion is the absence of intergranular fissures at the specified magnification. All boiling-acid work involving hydrofluoric acid and concentrated nitric or sulfuric acid must be performed under laboratory-grade ventilation with appropriate personal protective equipment by trained personnel.

Applications

Intergranular corrosion testing supports material qualification and integrity assurance across many industries:

  • Verification of solution annealing and stabilization heat treatments during stainless steel production
  • Welding procedure qualification and heat-affected zone evaluation for fabrications
  • Incoming material inspection and supplier certification against purchase specifications
  • Material selection and fitness-for-service assessment for chemical processing, petrochemical, refining, and fertilizer plants
  • Nuclear power components, where sensitization of piping and internals is a long-term aging concern
  • Pharmaceutical, food, and beverage equipment where product-contact surfaces must remain corrosion resistant
  • Failure analysis of components that have cracked in service, distinguishing intergranular corrosion from stress corrosion cracking or other mechanisms
  • Research and development of new low-carbon, stabilized, and high-nitrogen stainless grades

FAQ

What is the difference between the Huey test and the Strauss test?

The Huey test (ASTM A262 Practice C) exposes specimens to boiling 65% nitric acid for five 48-hour periods and evaluates results by corrosion rate, making it sensitive to carbides, sigma phase, and inclusions. The Strauss test (Practice E) exposes specimens to boiling copper–copper sulfate–sulfuric acid for about 24 hours and evaluates results by a 180° bend test for fissures. The Huey test is the more severe and quantitative method, while the Strauss test best simulates sulfur-containing service environments.

Can the oxalic acid etch test be used alone for acceptance?

No. The oxalic acid etch test is a rapid screening method. A ditch structure indicates possible susceptibility and must be confirmed by an appropriate immersion test such as Practice B, C, or E. Only step or conditionally acceptable dual structures may be used to accept material without further testing, as permitted by the governing specification.

Which test method is suitable for 316 or 316L stainless steel?

For molybdenum-bearing austenitic grades, the ferric sulfate–sulfuric acid test (Practice B), the copper–copper sulfate–50% sulfuric acid test (Practice F), or the nitric–hydrofluoric acid test (GB/T 4334.4) are commonly applied. The applicable method should be selected according to the product specification and the intended service environment.

When is a sensitizing heat treatment required before testing?

A sensitizing treatment, such as 650 °C for 2 hours or the ISO 3651 treatment of 700 °C for 30 minutes with water quenching, is applied when the specification requires evaluation of the material's intrinsic resistance in the sensitized condition—for example, for low-carbon or stabilized grades in the annealed delivery state. Weldments are generally tested in the as-welded condition.

What are typical acceptance criteria?

For immersion tests, acceptance is a maximum average corrosion rate (and sometimes a maximum single-period rate for the Huey test) defined by the material specification. For the Strauss-type tests, acceptance is the absence of cracks or fissures on the tension surface of the bent specimen at the specified magnification.

How long does intergranular corrosion testing take?

The oxalic acid etch test is completed within minutes, the Strauss test typically requires 24 hours of exposure plus bending and examination, the ferric sulfate test requires 120 hours, and the Huey test requires 240 hours of exposure across five boiling periods. Additional time is needed for specimen preparation, sensitizing treatments where specified, and reporting.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing