Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Corrugated Base Paper Standard Testing: Key Test Items, Methods and Applicable Standards

Corrugated base paper, also known as corrugating medium, is the fluted core layer of corrugated board and its compressive performance directly determines the stacking strength and transport safety of packaging boxes. Standard testing of corrugated base paper in accordance with GB/T 13023 and internationally recognized ISO test methods covers grammage, moisture content, bursting strength, Concora medium test (CMT), and short-span compression strength (SCT). This article provides a comprehensive overview of the sampling requirements, test items, testing methods, applications, and frequently asked questions related to corrugated base paper quality evaluation.

Technical Overview

Corrugated base paper, commonly referred to as corrugating medium, is an unbleached or semi-bleached kraft-type paper that is passed through corrugating rolls to form the fluted (arched) layer sandwiched between linerboards in corrugated fibreboard. The fluted structure acts as the structural backbone of the board, providing rigidity, vertical compression resistance, and cushioning performance for transport packaging.

Because the medium contributes a large proportion of the edge crush and stacking strength of finished corrugated boxes, its quality must be strictly controlled. In China, the governing product standard is GB/T 13023, which classifies corrugating medium into quality grades and specifies requirements for grammage tolerance, bursting strength, flat crush resistance of the fluted medium (CMT), and moisture content, with nominal grammages typically ranging from approximately 80 g/m² to 200 g/m². Internationally, equivalent laboratory test methods are published by ISO, allowing results from different markets to be compared on a consistent basis.

Standard testing of corrugated base paper is carried out by mill quality laboratories, converting plants, and accredited third-party laboratories for purposes such as lot release, incoming inspection, supplier qualification, product certification, and trade arbitration.

Testing Samples

Roll and Sheet Samples

Test material may be submitted as production rolls, full-width roll strips, or cut sheets of corrugating medium. Samples must be representative of the lot and free from defects such as wrinkles, breaks, water damage, edge crushing, and visible contamination, as these conditions can invalidate strength results.

Sampling Procedures

Sampling is performed in accordance with ISO 186 or GB/T 450. A statistically appropriate number of units is selected from the lot, and specimens are taken from positions distributed across the full width of the paper web, avoiding the outer wraps of rolls where moisture and mechanical damage are most likely. Specimens are cut cleanly with sharp instruments, and the machine direction (MD) and cross direction (CD) of every specimen are clearly marked, since compressive and tensile properties are strongly directional.

Conditioning Requirements

Paper properties are highly sensitive to humidity and temperature. All specimens must be preconditioned and conditioned to equilibrium in the standard atmosphere defined by ISO 187 or GB/T 10739, i.e., 23 °C ± 1 °C and 50 % ± 2 % relative humidity, before physical testing. Testing outside this atmosphere can cause significant deviation in grammage, burst, CMT, and SCT results.

Testing Items

Typical test items for corrugated base paper include physical strength properties, structural parameters, and chemical or optical characteristics, as listed below.

  • Grammage (basis weight), in g/m², and grammage tolerance
  • Thickness and apparent density
  • Moisture content at delivery
  • Bursting strength and burst index
  • Concora medium test (CMT), including CMT0 and CMT30
  • Short-span compression strength (SCT) in both machine and cross directions
  • Transverse compressive strength (ring crush method, RCT)
  • Tensile strength, tensile index, and breaking length
  • Water absorptiveness (Cobb value)
  • Ash (filler) content
  • Brightness (diffuse reflectance factor)
  • pH value of aqueous extract
  • Surface roughness or smoothness, where required

Testing Methods

Grammage and Thickness

Grammage is determined by weighing conditioned specimens of accurately known area in accordance with ISO 536 or GB/T 451.2. Thickness is measured under a defined static pressure using ISO 534 or GB/T 451.3, and apparent density is calculated as grammage divided by thickness. These values govern grade classification and are the basis for the index values used in strength specifications.

Moisture Content

Moisture content is determined by oven drying at 105 °C ± 2 °C to constant mass in accordance with ISO 287 or GB/T 462. Delivery moisture for corrugating medium is commonly specified around 8 %, and deviations affect both runnability on the corrugator and measured strength values.

Bursting Strength

Bursting strength is measured by clamping the specimen over a circular diaphragm and applying increasing hydraulic pressure until rupture, following ISO 2758 or GB/T 454. The burst index, expressed in kPa·m²/g, normalizes bursting strength against grammage and is a core acceptance criterion in GB/T 13023.

Concora Medium Test (CMT)

The CMT measures the flat crush resistance of the medium after laboratory fluting and is the most characteristic test for corrugating medium. Specimens are fluted in a laboratory fluting device and compressed between parallel platens, either immediately after fluting (CMT0) or after a 30-minute recovery period (CMT30), as specified in ISO 7263 or GB/T 2679.6. CMT results correlate strongly with the flat crush performance of the finished board and the vertical load-bearing capacity of boxes.

Short-Span Compression Strength (SCT)

SCT is determined by compressing a short strip of paper over a span of only 0.7 mm in accordance with ISO 9895 or GB/T 2679.10. The very short gauge length minimizes buckling and isolates the intrinsic fiber-to-fiber bonding strength. SCT, particularly in the cross direction, is widely used to predict the edge crush strength of corrugated board and therefore the ultimate box compression strength.

Transverse Compressive Strength (Ring Crush Method)

Where specified, the compressive strength of the medium is measured using a ring-supported specimen in accordance with ISO 12192. This method has traditionally been used for grammage-based grade tables and remains a common acceptance parameter for medium-grade verification.

Tensile Properties

Tensile strength, elongation, and tensile energy absorption are measured with a constant-rate-of-extension tensile tester in accordance with ISO 1924-2 or GB/T 12914, in both machine and cross directions. Breaking length provides a grammage-independent measure of the tensile quality of the furnish.

Water Absorptiveness (Cobb Value)

Water absorptiveness is determined by exposing one surface of the specimen to water for a defined contact time (typically 60 seconds) and measuring the mass of water absorbed per unit area, following ISO 535 or GB/T 1540. This indicates the degree of sizing and influences glueability and performance under humid transport conditions.

Chemical and Optical Properties

Ash content is determined by igniting the specimen at the specified temperature in accordance with ISO 2144 or GB/T 742 and reflects the mineral filler or recycled ash level. The pH of the cold aqueous extract is measured per ISO 6588-1 or GB/T 1545, and brightness is determined by diffuse reflectance measurement per ISO 2470 or GB/T 7974 where optical appearance is contractually specified.

Applications

Standard testing of corrugated base paper supports quality assurance and decision-making throughout the packaging supply chain.

  • Mill process control and product release testing for corrugating medium production lines
  • Incoming material inspection and supplier qualification at corrugated box and board converting plants
  • Verification of grade claims and compliance with GB/T 13023 or contractual technical agreements
  • Prediction of downstream board performance, including edge crush strength and box compression strength, through SCT and CMT data
  • Input data for performance-oriented packaging design, including export packaging and dangerous goods packaging systems
  • Research and development of recycled fiber formulations, refining strategies, and sizing programs
  • Failure analysis of box compression or flute collapse complaints, and independent arbitration in trade disputes conducted by accredited third-party laboratories

FAQ

Which standard governs corrugated base paper in China?

GB/T 13023 is the Chinese national product standard for corrugated base paper. It defines product grades, grammage series, and the required values for key indicators such as bursting strength, flat crush resistance of the fluted medium, and moisture content, together with the corresponding test method standards.

What is the difference between CMT and SCT?

CMT evaluates the flat crush resistance of the paper after it has actually been fluted, so it reflects both fiber strength and flute formability. SCT measures the intrinsic compressive strength of an unfluted strip over a 0.7 mm span and is a faster, more fundamental indicator. Both correlate with finished board performance, and many specifications require both values.

What do CMT0 and CMT30 mean?

CMT0 is measured immediately after laboratory fluting, while CMT30 is measured after the fluted specimen has recovered for 30 minutes. CMT30 is generally the contractually specified value because it better represents the strength of the medium after fluting and bonding on a corrugator.

Why is conditioning so important?

Paper strength and moisture content change significantly with ambient humidity. Testing all specimens in the standard atmosphere of 23 °C ± 1 °C and 50 % ± 2 % relative humidity, per ISO 187 or GB/T 10739, ensures that results are reproducible and comparable between laboratories.

Which properties best predict box stacking strength?

Cross-direction SCT and CMT of the medium, combined with linerboard compression values, are the strongest predictors of the edge crush strength of corrugated board and, in turn, the box compression strength. Moisture content and Cobb value are also monitored because humid conditions degrade field performance.

Can recycled corrugating medium be tested using the same standards?

Yes. The test methods are fiber-source independent, and recycled-based medium is evaluated against the same ISO and GB/T methods. Grade classification is determined by the measured results rather than the fiber furnish, although ash content and pH tests are often added for recycled grades.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing